Crystallinity Fraction Calculator (DSC)

Find the percent crystallinity of a semicrystalline polymer from DSC enthalpies with cold crystallization and filler corrections, or from density.

🔬 Crystallinity Fraction Calculator (DSC)
Polymer preset for the reference enthalpy (illustrative)
Melting enthalpy (ΔHm)
J/g
Cold crystallization (ΔHcc)
J/g
100% crystalline (ΔHm0)
J/g
Filler weight fraction (w)
wt %
Reference density preset (illustrative)
Sample density (ρ)
g/cm³
Amorphous density (ρa)
g/cm³
Crystalline density (ρc)
g/cm³
Crystallinity (Xc)
—
Amorphous fraction
—
Net enthalpy (ΔHm - ΔHcc)
—
Net per gram of polymer
—
Xc without cold crystallization
—
Reference enthalpy used
—

Crystallinity by mass
—
Crystallinity by volume
—
Amorphous fraction (mass)
—
Factor ρc/ρ
—
Density span ρc - ρa
—
Position between ρa and ρc
—

🔬 What is the Crystallinity Fraction of a Polymer?

Most polymers that crystallize are only semicrystalline. Ordered lamellae, where chain segments pack in a regular lattice, are embedded in disordered amorphous regions, and the chains pass through both. The crystallinity fraction Xc is the share of the material that is in the ordered phase, expressed as a percentage by mass or by volume. It matters because the crystalline part is stiffer, denser, less permeable and melts at a higher temperature than the amorphous part. Stiffness, yield strength, barrier properties, clarity and shrinkage of polyethylene, polypropylene, PET, nylon and PLA parts all follow crystallinity closely, and it changes with cooling rate, annealing and additives.

Differential scanning calorimetry (DSC) is the most common way to measure it. The sample is heated at a fixed rate and the heat flow is integrated over the melting endotherm to give the enthalpy of fusion ΔHm in J/g. Dividing by the enthalpy of fusion of a hypothetical 100 percent crystalline sample, ΔHm0, gives the crystalline share. Two corrections are routine. If the scan shows an exotherm before melting, as in quenched PET or PLA, that cold crystallization enthalpy ΔHcc was released by crystals formed during the scan and is subtracted. If the sample contains filler, glass fibre or pigment, the measured enthalpy is divided by the polymer weight fraction 1 - w so that it is expressed per gram of polymer. The full expression is Xc = (ΔHm - ΔHcc) / (ΔHm0 (1 - w)) × 100.

The calculator also offers the density method. Because crystals pack more tightly than the amorphous phase, the sample density lies between an amorphous density ρa and a crystalline density ρc. The volume fraction is (ρ - ρa)/(ρc - ρa), and multiplying by ρc/ρ gives the mass fraction. Both methods rest on reference values that depend on the source, so the presets are labelled illustrative and you should replace them with the figures that match your polymer and protocol. After you have the crystallinity, the melting temperature depression calculator shows how comonomer, diluent and lamella thickness lower the melting point, and the Fox equation estimator covers the amorphous side of the same thermogram.

📐 Formula

Xc  =  (ΔHm − ΔHcc) ÷ (ΔHm0 (1 − w))  ×  100
Xc = crystallinity of the polymer phase (percent by mass)
ΔHm = measured enthalpy of melting (J/g of sample)
ΔHcc = enthalpy of cold crystallization measured during heating (J/g), 0 if none
ΔHm0 = enthalpy of fusion of the 100 percent crystalline polymer (J/g, a literature value)
w = filler weight fraction (percent divided by 100)
Example: ΔHm = 190 J/g, ΔHm0 = 293 J/g, no filler gives Xc = 190 / 293 = 64.85 %
Xv  =  (ρ − ρa) ÷ (ρc − ρa),    Xm  =  Xv ρc ÷ ρ
ρ = sample density (g/cm3); ρa = amorphous density; ρc = crystalline density
Xv = crystalline volume fraction; Xm = crystalline mass fraction
Example: ρ = 0.950, ρa = 0.855, ρc = 1.000 gives Xv = 65.52 % and Xm = 68.97 %

📖 How to Use This Calculator

Two methods

1
Choose DSC enthalpy or Density - Use DSC when you have integrated melting and, if present, cold crystallization peaks. Use Density when you have a measured sample density.
2
Pick a reference - The preset menu fills the 100 percent crystalline enthalpy or the reference densities with illustrative literature values. Type your own to override, which switches the preset to Custom.
3
Enter your measurements - Type ΔHm and ΔHcc in J/g and the filler weight percent, or the sample density in g/cm³.
4
Read Xc - The result shows percent crystallinity with the amorphous fraction and the value without the cold crystallization correction, and the chart marks your point on the Xc line.

💡 Example Calculations

Example 1 - Polyethylene with no cold crystallization

ΔHm = 190 J/g, ΔHcc = 0, ΔHm0 = 293 J/g, w = 0

1
Net enthalpy = 190 - 0 = 190.00 J/g and the polymer fraction is 1 - 0 = 1.
2
Xc = 190 / (293 × 1) × 100 = 64.85 %.
3
The amorphous fraction is 100 - 64.85 = 35.15 %.
Xc = 64.85 %, amorphous = 35.15 %
Try this example →

Example 2 - Quenched PET with cold crystallization

ΔHm = 40 J/g, ΔHcc = 25 J/g, ΔHm0 = 140 J/g (illustrative), w = 0

1
Net enthalpy = 40 - 25 = 15.00 J/g, the part that was crystalline before the scan.
2
Xc = 15 / 140 × 100 = 10.71 %.
3
Ignoring cold crystallization would give 40 / 140 = 28.57 %, nearly three times too high.
Xc = 10.71 % (28.57 % without the correction)
Try this example →

Example 3 - Filled polypropylene

ΔHm = 80 J/g, ΔHcc = 0, ΔHm0 = 207 J/g (illustrative), w = 20 wt %

1
The polymer weight fraction is 1 - 0.20 = 0.80, so the enthalpy per gram of polymer is 80 / 0.80 = 100.00 J/g.
2
Xc = 100 / 207 × 100 = 48.31 %.
3
Without the filler correction the answer would be 80 / 207 = 38.65 %, which would understate the polymer crystallinity.
Xc = 48.31 %, amorphous = 51.69 %
Try this example →

Example 4 - Polyethylene from density

ρ = 0.950 g/cm³, ρa = 0.855, ρc = 1.000

1
Volume fraction Xv = (0.950 - 0.855) / (1.000 - 0.855) = 0.095 / 0.145 = 65.52 %.
2
The conversion factor is ρc/ρ = 1.000 / 0.950 = 1.0526.
3
Mass fraction Xm = 65.52 % × 1.0526 = 68.97 %.
Xm = 68.97 % by mass, Xv = 65.52 % by volume
Try this example →

Example 5 - PET from density

ρ = 1.380 g/cm³, ρa = 1.335, ρc = 1.455 (illustrative)

1
Xv = (1.380 - 1.335) / (1.455 - 1.335) = 0.045 / 0.120 = 37.50 %.
2
Xm = 37.50 % × 1.455 / 1.380 = 39.54 %.
Xm = 39.54 % by mass
Try this example →

❓ Frequently Asked Questions

How do you calculate percent crystallinity from DSC?+
Integrate the melting endotherm to get dHm in J/g, subtract any cold crystallization exotherm dHcc, divide by the enthalpy of a fully crystalline sample dHm0 and by (1 - w) if filler is present, then multiply by 100. For dHm = 190 J/g and dHm0 = 293 J/g the result is 64.85 percent.
What is the enthalpy of 100 percent crystalline polyethylene?+
Literature values run from about 288 to 293.6 J/g depending on method. The calculator preset of 293 J/g is illustrative. Always quote the reference you used, since changing it from 293 to 288 raises the crystallinity by about 2 percent in relative terms.
Why subtract the cold crystallization enthalpy?+
Cold crystallization is crystallization that happens during heating in the DSC, for example when quenched PET or PLA crystallizes above its glass transition. The heat is released as an exotherm before the melt, so melting enthalpy alone overstates the crystallinity the sample had at the start.
How do I correct for filler or fibre content?+
Divide the enthalpy by the polymer weight fraction 1 - w. A composite with 20 percent filler and 80 J/g melting enthalpy has 100 J/g per gram of polymer, so with a 207 J/g reference the crystallinity is 48.31 percent, not 38.65 percent.
What is the density method for crystallinity?+
The density of a semicrystalline polymer lies between the amorphous density rho_a and the crystalline density rho_c. The volume fraction is (rho - rho_a)/(rho_c - rho_a), and the mass fraction multiplies it by rho_c/rho. For polyethylene at 0.950 g/cm3 the mass crystallinity is 68.97 percent.
Which is larger, mass or volume crystallinity?+
Mass crystallinity is larger because crystalline regions are denser than amorphous ones. The factor between them is rho_c/rho, which exceeds 1 for any partially crystalline sample, so 65.52 percent by volume corresponds to 68.97 percent by mass in the polyethylene example.
How accurate is DSC crystallinity?+
Typical uncertainty is several percent of the crystallinity. Baseline choice, heating rate, reorganisation during the scan, the assumed reference enthalpy and the weight of the sample all contribute. Comparing samples measured with the same protocol is more reliable than comparing absolute values.
Does the reference enthalpy depend on temperature?+
Yes. The heat of fusion of a perfect crystal depends on the melting temperature, and some references correct it with the heat capacity difference. The calculator uses a single constant value, which is the common practical convention, and flags it as illustrative.
Can crystallinity be above 100 percent?+
It should not. A value above 100 percent signals a reference enthalpy that is too low for your polymer, a baseline that includes other transitions, or a filler fraction entered incorrectly. Check the integration limits and the weight fractions first.
Is DSC crystallinity the same as X-ray crystallinity?+
Not exactly. DSC measures heat of fusion, density measures packing and X-ray diffraction measures ordered lattice scattering, so the three can differ by several percent for the same sample because of defects and the definition of the interface region between crystal and amorphous phases.

📚 Sources and Notes

The filler-corrected form of the DSC crystallinity, Xc = ΔHm / ((1 - φ) ΔHm0) × 100, appears in a polypropylene composite study on arXiv. Reported 100 percent crystalline polyethylene enthalpies near 288 J/g from combined DSC and X-ray work are discussed in this thermal analysis paper, and the density method with amorphous and crystalline densities is outlined in the ScienceDirect Topics overview of amorphous density. Combining the cold crystallization subtraction with the filler correction is the common practical reading of these sources, and should be checked against the standard your laboratory follows. The presets for polyethylene (293 J/g), polypropylene (207 J/g), PET (140 J/g) and PLA (93 J/g) and the reference densities are illustrative values that differ between publications, for example 165 to 207 J/g for polypropylene, so replace them with the figures you cite.

See also the polymer physics calculators.

How do you calculate percent crystallinity from DSC?

Integrate the melting endotherm to get dHm in J/g, subtract any cold crystallization exotherm dHcc, divide by the enthalpy of a fully crystalline sample dHm0 and by (1 - w) if filler is present, then multiply by 100. For dHm = 190 J/g and dHm0 = 293 J/g the result is 64.85 percent.

What is the enthalpy of 100 percent crystalline polyethylene?

Literature values run from about 288 to 293.6 J/g depending on method. The calculator preset of 293 J/g is illustrative. Always quote the reference you used, since changing it from 293 to 288 raises the crystallinity by about 2 percent in relative terms.

Why subtract the cold crystallization enthalpy?

Cold crystallization is crystallization that happens during heating in the DSC, for example when quenched PET or PLA crystallizes above its glass transition. The heat is released as an exotherm before the melt, so melting enthalpy alone overstates the crystallinity the sample had at the start.

How do I correct for filler or fibre content?

Divide the enthalpy by the polymer weight fraction 1 - w. A composite with 20 percent filler and 80 J/g melting enthalpy has 100 J/g per gram of polymer, so with a 207 J/g reference the crystallinity is 48.31 percent, not 38.65 percent.

What is the density method for crystallinity?

The density of a semicrystalline polymer lies between the amorphous density rho_a and the crystalline density rho_c. The volume fraction is (rho - rho_a)/(rho_c - rho_a), and the mass fraction multiplies it by rho_c/rho. For polyethylene at 0.950 g/cm3 the mass crystallinity is 68.97 percent.

Which is larger, mass or volume crystallinity?

Mass crystallinity is larger because crystalline regions are denser than amorphous ones. The factor between them is rho_c/rho, which exceeds 1 for any partially crystalline sample, so 65.52 percent by volume corresponds to 68.97 percent by mass in the polyethylene example.

How accurate is DSC crystallinity?

Typical uncertainty is several percent of the crystallinity. Baseline choice, heating rate, reorganisation during the scan, the assumed reference enthalpy and the weight of the sample all contribute. Comparing samples measured with the same protocol is more reliable than comparing absolute values.

Does the reference enthalpy depend on temperature?

Yes. The heat of fusion of a perfect crystal depends on the melting temperature, and some references correct it with the heat capacity difference. The calculator uses a single constant value, which is the common practical convention, and flags it as illustrative.

Can crystallinity be above 100 percent?

It should not. A value above 100 percent signals a reference enthalpy that is too low for your polymer, a baseline that includes other transitions, or a filler fraction entered incorrectly. Check the integration limits and the weight fractions first.

Is DSC crystallinity the same as X-ray crystallinity?

Not exactly. DSC measures heat of fusion, density measures packing and X-ray diffraction measures ordered lattice scattering, so the three can differ by several percent for the same sample because of defects and the definition of the interface region between crystal and amorphous phases.